E-Mobility Engineering 018 l In conversation: Asher Bennett l Cake Kalk OR e-bike dossier l Battery management systems focus l Rare earth and magnet-free motors insight l Eive electric 2CV van digest l Anode materials insight l Automotive biometrics focus

such as Si0 x can be used with graphite up to 10% and don’t take into account the expansion; that is in production now,” he adds. “The second generation is engineered materials that take expansion into account by introducing porosity, and usually that’s a composite material. The third generation is the all- silicon approach with silicon nanowires on copper substrates. “We think Gen3 requires a lot of investment in processing, it’s a slow process and it doesn’t scale. So we have focused on the first and second- generation processes, which we call NSP1 and NSP2. We have licensed NSP1 exclusively to SK Chemicals, who are scaling up to supply the market this year and in 2024, and we have moved some of our customers over to them. “NSP1 has advantages over a pure Si0 x process, which has oxygen that reacts with lithium ions with a first-cycle loss and a drop in capacity. That means having extra cathode material in the battery, which is expensive. “Our NSP1 material has much lower oxygen levels so the initial loss is lower. We take silicon, mill it to nanoscale and spray-dry it to create a larger secondary particle in a carbon matrix. We use metallurgical-grade silicon powders, and in our case 99% purity is fine so there is a good supply chain.” Nexeon is scaling up production for its NSP2 material. This uses silicon from silane gas deposited on a porous carbon substrate. “The carbon is a very porous material, and the total pore volume, and size and distribution of the pores, are important factors, and that’s what we optimise,” Dr Brown says. “The substrate is engineered activated carbon, and we deposit the silicon into the carbon pores. The final material is about 50% silicon and 50% carbon, so the capacity is around 2000 Ah/kg, as we need to leave enough space for the silicon to expand into.” This approach avoid problems with the lithium ions plating the silicon. In tests it supports safe charging to 80% capacity in 15 minutes. “Perfect porosity would mean there is 0% swelling at the particle level rather than 300%, but we are at less than half the theoretical limit and we have customers using that level of NSP2 without any problems,” says Dr Brown. The availability of silane, which is also used for silicon nanotube processes, is a potential issue as production scales up. “Most of the silane currently produced goes into solar cells, but its producers see an opportunity to expand and diversify, and we are in talks about supply,” says Dr Brown. The process also takes place at a lower temperature than that for graphite, which is key given the high cost of energy. “We don’t use vacuum and we do not go above 500 oC, so it’s a relatively straightforward process and its scales very well from a process time perspective,” says Dr Brown. “In principle it can be a continuous process, which is more efficient, but there is middle ground. A batch process can be semi-continuous with short batch times and minimal loading and unloading times with cooling/heating, so you can call it semi-continuous.” Another key feature of the process is that thewaste product is hydrogen, which can be used for its thermal properties in clean technology applications or returned to the silane producer. Ionic MT has a process that produces silicon nanoparticles that are used for making nanotubes less than 150 nm long (Courtesy of Ionic MT) 62 March/April 2023 | E-Mobility Engineering Deep insight | Anode materials

RkJQdWJsaXNoZXIy MjI2Mzk4