E-Mobility Engineering 018 l In conversation: Asher Bennett l Cake Kalk OR e-bike dossier l Battery management systems focus l Rare earth and magnet-free motors insight l Eive electric 2CV van digest l Anode materials insight l Automotive biometrics focus
grid you want for the graphite, so you have to run above 2200 oC where the grid is settling, but we have to go higher for thinner layers. The energy flow to each particle is more controllable so there is more consistency from particle to particle.” This is different from composite anodes that combine other materials with the graphite. “Composite materials typically have a different processing route,” says Weiand. “Most are a silicon carbon composite, where you start with carbon and then synthesise to a composite or start with silicon. “We have seen both being successful – we don’t see the real performance data of the cell later on [as that is tested by the customer] so we can’t compare the materials, but we have built equipment for both routes. Everyone is working on different ideas on how the composite can be created. “We do both carbon and silicon process development, and we have our own test centre to demonstrate the structures of thematerial. We are not developing the process but we can take the process ideas that customers have and scale themup with testing. We can do almost any process – not just silicon but other metal-based compositematerials.” Coating the anode is another issue for the process. Particles in the anode, particularly silicon, can be coated with carbon to form a composite. “The coating can come froma liquid such as pitch that is then later run through a pyrolyser – that’s one route,” says Weiand. “But a lot of material is released from that process as gases. You can also have coating processes using carbon- carrying gases deposited on thematerial. The driver is not the pure efficiency of the process but the properties our customers want to achieve.” Silicon Silicon is an increasingly popular material for anodes, as it has a much higher energy density than graphite, with the potential for 4200 mAh/g to create cells with a density of up to 800 Wh/litre. However, it swells in size when it takes on the energy from the lithium ions. This swelling, which can be as much as 300%, can cause the cell to split, releasing the lithium electrolyte and potentially catching fire. It can be managed though in flexible pouch cells at the cost of the overall energy density, but causes problems with the more rigid cylindrical cell designs. Silicon dioxide has been the initial material used for anodes but in low quantities to avoid the swelling problem. “The appetite for silicon is there and getting stronger, and we can see that in customers testing and qualifying materials with demand forecasts, so it’s just a question of by howmuch and how quickly this demand will grow,” says Dr Scott Brown, CEO of Nexeon. “The first-generation materials “There are plenty of graphitemines but the properties and energy efficiencies of the rawmaterial fromeachmine differ, and with energy prices rising it is more difficult to produce artificial graphite,” he says. “Artificial carbons open up new approaches with other structures of carbon as a drop-inmaterial.” One approach uses an oil-based coke called petrocoke in a batch process where the coke is the electrode. Carbon black is put over the coke and high power to heat to 3000 oC, then the graphitisation settles into layers of graphite in a grid. “By varying the temperature we can influence the grid distance [the distance between the layers of carbon] and that is the performance criteria for the anode,” Weiand says. “Controlling the process precisely is not easy though, so it is based on a blend of materials. “The temperature is defined by the Nexeon is collaborating with solid-state battery technology company Ilika to develop a solid- state battery using a silicon anode (Courtesy of Nexeon) March/April 2023 | E-Mobility Engineering 61 Deep insight | Anode materials
Made with FlippingBook
RkJQdWJsaXNoZXIy MjI2Mzk4