E-Mobility Engineering 018 l In conversation: Asher Bennett l Cake Kalk OR e-bike dossier l Battery management systems focus l Rare earth and magnet-free motors insight l Eive electric 2CV van digest l Anode materials insight l Automotive biometrics focus

Lithiummetal anodes in reality with all the inactive materials these carbon matrix based Si products are only an incremental improvement over SiOx. Paraclete’s use of a Polymer matrix’s enables over 70% active Si material thereby greater than 2500mAh/g of active Si material equating to over 1900 Wh/kg battery With Paraclete, no longer is there a limit to 12% silicon, an incremental Improvement to SiOx but with Paraclete’s polymer matrix, nearly 8x the improvement over graphite. “We use a polymer matrix –we can use any source of silicon, whether mined or solar grade,” said JeffNorris, founder and CEOof Paraclete. This startswith a 150nm diameter silicon particle in a polymer spherewith a diameter of 5 to 7um. “We put a polymer matrix around the silicon which gives it elasticity with self-healing. The architecture handles swelling in the polymer and stops the electrolyte getting in,” he said. “We allow the silicon to expand as we put an artificial SEI around the silicon to create a primary particle. Then we place that in a non-silicon silo shell which is ionic and conductive on top of the polymer matrix so that the electrolyte forms the SEI on the silo shell.” This isbeingused for anodeswith25% andgreater silicon togiveexistingbattery packs a rangeof up to 1000km, saysNorris. “Our customers are routinely achieving 1000 cycles because of the polymer and the electrolyte is not consumed,” said Norris, “We started testing with customers late 2021 and some customers are in their third or fourth cycle of optimisation for performance. Each cathode has a different voltage range and traditionally you need tomatch that with the graphite and the silicon. That’s not necessary with our silicon as we’ve taken out the carbonisation stage and that means we don’t need themassive manufacturing infrastructure.” Using a polymer is a low temperature (sub500degreeC), lowwaste process that can be installed at the battery cell Using lithium as the anode has even higher theoretical energy density than silicon, but there are major challenges. One is a gap in the supply chain for next-generation batteries for high-performance anode materials, says Maciej Jastrzebski, co- founder and CEO of Li-Metal. “On the one hand the technology is starting to get to the point of being taken seriously with testing for EVs, but on the other there is a gap in metal production and understanding the drawbacks, and coupling that with a production process for low-cost anodes,” he says. Between 7000 and 20,000 tonnes of battery-grade metal will be needed by 2030; the industry currently has a capacity of 7000 t of nominal capacity, with half of that used for batteries. The lithium is produced from lithium chloride via lithium carbonate from brine, or lithium sulphate from rocks, but the latter needs to be refined to lithium carbonate and then turned back into the chloride. “This creates an upstream problem, so the challenge is to turn the carbonate feedstock into metal,” Jastrzebski says. “We are therefore looking at taking lithium carbonate and turning it into the chloride as a precursor.” Current production uses a rolling process, extruding the lithium into a foil 200-300 microns thick. There is a problem, however, in that keeping the foil from breaking or splitting becomes harder as the foil gets thinner, and is harder still as the lithium metal itself is weak. “You can cut it with a knife, so the problem of rolling the material is profound,” Jastrzebski says. “It ends up much thicker than you want it to be, and you are forced to build the cells using thin strips of lithium.” One of the challenges is the need to minimise the inclusions in the metal, as they create splits in the foil. “That forces people into strange-size formats, and I see rolling as a dead-end technology,” he says. “You are composing the anode to make the rolling as easy as possible, which constrains the anode’s performance.” Li-Metal has therefore developed a process using vacuum-based physical vapour deposition (PVD), similar to that used for the thin metallic coatings on bags of potato crisps. “What attracted us to this approach are the economics and commercial availability of the equipment as a manufacturing platform,” Jastrzebski says. “The other, less appreciated Lithiummetal anodes are currently produced using a rolling process (left), which causes problems, so Li-Metal has switched to vacuum-based physical vapour deposition (Courtesy of Li-Metal) 64 March/April 2023 | E-Mobility Engineering

RkJQdWJsaXNoZXIy MjI2Mzk4